<listing id="b1vrb"><cite id="b1vrb"></cite></listing>
<var id="b1vrb"></var>
<ins id="b1vrb"><span id="b1vrb"></span></ins>
<var id="b1vrb"></var>
<var id="b1vrb"><video id="b1vrb"><thead id="b1vrb"></thead></video></var>
<var id="b1vrb"><strike id="b1vrb"><listing id="b1vrb"></listing></strike></var>
<cite id="b1vrb"></cite>
<ins id="b1vrb"><span id="b1vrb"></span></ins>
<thead id="b1vrb"></thead><menuitem id="b1vrb"></menuitem>
<var id="b1vrb"></var>
<var id="b1vrb"></var>
<var id="b1vrb"></var>
<var id="b1vrb"><strike id="b1vrb"></strike></var>
<cite id="b1vrb"><strike id="b1vrb"><listing id="b1vrb"></listing></strike></cite>
<cite id="b1vrb"><video id="b1vrb"></video></cite>
Volume 32 Issue 6
Aug.  2021
Turn off MathJax
Article Contents
ZHANG Li-min, LIU Jun-bo, SUN Dong-bo, WANG Shu-ming. Microstructure and failure analysis of Fe-Ni based alloy rollers produced by plasma cladding[J]. Chinese Journal of Engineering, 2010, 32(6): 777-781. doi: 10.13374/j.issn1001-053x.2010.06.014
Citation: ZHANG Li-min, LIU Jun-bo, SUN Dong-bo, WANG Shu-ming. Microstructure and failure analysis of Fe-Ni based alloy rollers produced by plasma cladding[J]. Chinese Journal of Engineering, 2010, 32(6): 777-781. doi: 10.13374/j.issn1001-053x.2010.06.014

Microstructure and failure analysis of Fe-Ni based alloy rollers produced by plasma cladding

doi: 10.13374/j.issn1001-053x.2010.06.014
  • Received Date: 2009-09-21
  • Fe-Ni based high temperature wear-resistant powder was cladded on 45# round steel to obtain an Fe-Ni based alloy roller by plasma cladding.Scanning electric microscope,energy spectrometer and X-ray diffractometer were adopted to study the microstructure of the Fe-Ni based alloy coating and the failure surface of the Fe-Ni based alloy roller.It is shown that the morphology of the Fe-Ni based high-temperature wear-resistant coating is well and the morphology is planar crystal at the coating-substrate bonding,while the morphology becomes dendrite at the middle and the top of the coating.The γ-(Fe,Ni) content reduces following the bottom-middle-top order in the coating,but the (Cr,Fe)7C3 is just the opposite.The failure mechanism of the Fe-Ni based alloy roller is thermal fatigue cracking and grain wear.

     

  • loading
  • 加載中

Catalog

    通訊作者: 陳斌, bchen63@163.com
    • 1. 

      沈陽化工大學材料科學與工程學院 沈陽 110142

    1. 本站搜索
    2. 百度學術搜索
    3. 萬方數據庫搜索
    4. CNKI搜索
    Article views (141) PDF downloads(7) Cited by()
    Proportional views
    Related

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return
    Return
    青青草原综合久久大伊人精品